Slumping for Camera Cases

I am not skilled at slumping. Shallow things are fine, but I need to practice more with deeper shapes.

I tried in kiln 2, it didn't work past about 30 degrees.  Switched to kiln 1.

Fired at 11:00, 20131119



Program: 
  1. 150* to 300* hold 00:00
  2. 250* to 638* hold 00:10
  3. 999 to 482* hold 01:00
  4. 55* to 371* hold 00:00
  5. 999 to 50* hold 00:00
  6. End
I came in at 2:30 to check and gradually moved the temperature up to 680. The results were not the best, but it will do, I think.